Why Do Zirconia Crowns Crack During Sintering?

Nov 24, 2026|

Mr. Wang
Mr. Wang
Position: R&D Engineer Expertise: Dental CAD/CAM systems, zirconia applications, sintering technology, dental equipment development Experience:17 years in dental product research and manufacturiover Focus Areas: product research,technical improvement

Why Do Zirconia Crowns Crack During Sintering?

 

4

A zirconia crown can look perfectly normal after milling and still develop a crack during sintering. In some cases, the crack becomes visible as soon as the crown is removed from the furnace. In others, it is not noticed until staining, polishing, or fitting.

When this happens, the furnace is often the first thing the laboratory checks. The sintering program may be changed, the temperature reduced, or the heating rate adjusted. Sometimes these changes help, but they do not explain every failure.

From a manufacturing and materials perspective, a crack discovered after sintering does not necessarily mean that it originated inside the furnace. A small defect may already have been present in the zirconia blank or introduced during milling. The sintering process may make an existing defect easier to detect or allow it to develop into a larger fracture.

A proper investigation needs to consider the entire production route: the zirconia blank, CAD/CAM machining, handling before sintering, and the thermal process itself.

1. A Crack Found After Sintering May Have Started Much Earlier

The first question I would ask is not simply, "What was the sintering temperature?" I would ask, "At which stage could the crack have started?"

There are several possibilities:

During the manufacturing of the zirconia blank

During milling, particularly around thin or difficult-to-machine areas

During removal of the restoration from the disc

During cleaning, adjustment, or handling before sintering

During the thermal process, when an existing defect develops further

These possibilities need to be distinguished because each requires a different corrective action.

For example, changing a furnace program will not remove a crack caused by a damaged milling bur. Replacing a zirconia disc will not solve a recurring problem caused by excessive tool wear or an unsuitable machining strategy.

There is also a difference between a visible crack and a microcrack. A microcrack may be too small to detect under normal laboratory lighting. It may only become visible after further processing or when the restoration eventually breaks.

A crown can therefore pass a quick visual inspection after milling and still fail later in the workflow.

2. Milling Can Introduce Small Defects That Become Larger Problems

CAD/CAM milling is one of the first areas I would investigate when a laboratory reports repeated cracks after sintering.

Partially sintered zirconia is easier to machine than fully dense zirconia, but machining can still cause mechanical damage. Cutting tools apply forces to the material as they remove it. Depending on the tool condition, cutting parameters, tool path, and local geometry, small chips or cracks may form on the surface.

A study published in Dental Materials in 2004 investigated machining-related damage in Y-TZP zirconia. The researchers simulated the grinding of internal crown surfaces and observed surface flaws and microcracks. The measured crack lengths ranged from approximately 2 to 15 μm.

These defects are much smaller than those a technician would normally notice during a visual inspection. However, the findings show that machining can introduce damage on a scale that is not visible to the naked eye.

The study also found that the diamond tool itself was an important factor. The number and shape of active diamond grains affected the machining process. The appearance of a finished crown alone is therefore not enough to assess milling quality.

A restoration may have a smooth-looking surface but still contain subsurface damage.

What should a laboratory check?

If cracks appear repeatedly after milling and sintering, I would first check:

Bur condition: Are the diamond-coated tools worn, chipped, or being used beyond their recommended service life?

Tool replacement records: Does the laboratory record the number of milling hours or restorations processed by each bur?

Machining strategy: Are the feed rate, cutting depth, and tool paths appropriate for the zirconia material and restoration geometry?

Internal surface quality: Are there visible scratches, small chips, or irregular marks around the intaglio surface?

Machine condition: Is the spindle running smoothly, and are the tool holders and clamping system in good condition?

One useful troubleshooting method is to compare restorations produced with a new bur against those produced with a bur near the end of its service life. Keep the material batch, design, and machining program unchanged. If the results differ consistently, tool condition deserves further investigation.

This comparison is more informative than changing several machine settings at the same time.

3. The Condition of the Zirconia Blank Matters

Not every defect originates in the dental laboratory. Some can develop much earlier, during powder preparation and blank production.

Zirconia discs are made through a series of powder-processing and forming steps. The powder needs to be distributed and compacted properly. If the particles are not packed uniformly, local density differences may remain in the pressed body.

These defects are not always visible on the outside of the blank.

A 2014 study by Zhao and colleagues investigated micro-defects and residual stresses introduced during different processing stages of zirconia dental restorations. The researchers compared several manufacturing routes, including green milling, raw milling, and grinding.

One finding was that large packing voids could remain inside the material even after cold isostatic pressing and sintering. Milling could remove some surface voids, but it could not eliminate defects located deeper inside the material.

The researchers also observed more serious chipping during raw milling than during green milling. They associated much of this chipping with existing packing voids and the brittle failure behavior of the material.

This has implications for both laboratories and distributors.

A zirconia disc can have a clean external appearance while still containing internal defects. Inspecting the disc surface alone cannot establish the quality of its internal structure.

What should buyers ask zirconia suppliers?

When evaluating a new zirconia supplier, buyers should ask about more than flexural strength and translucency values.

Useful questions include:

How is the zirconia powder prepared before pressing?

Is powder distribution controlled during production?

What pressing process is used?

Is cold isostatic pressing included?

How are density variations and internal defects monitored?

Does the manufacturer inspect finished discs before packaging?

Can the supplier provide batch traceability?

A supplier may publish a flexural strength value, but that single number does not describe every aspect of material consistency.

For a laboratory processing many restorations each day, batch-to-batch stability also matters. If one disc produces normal results while another from the same product range shows repeated defects, the supplier should investigate the production batch rather than simply recommend a different sintering program.

4. Thin Areas and Sharp Geometry Need More Attention

The restoration design is another possible source of cracking.

A crown does not have the same thickness everywhere. The occlusal surface, axial walls, marginal areas, connectors, and internal transitions all have different geometries.

When a restoration contains a very thin section, a sharp internal corner, or an abrupt change in thickness, local stress may become concentrated in that area.

These areas may also be more vulnerable during milling. A small amount of material damage around a thin margin or narrow connector can have a greater effect than a similar defect on a thicker, less critical surface.

For example, consider two zirconia bridges with the same overall length. One has smooth transitions and reasonably uniform connector dimensions. The other has narrow connectors and sharp internal transitions.

Even if both bridges are milled from the same disc and processed using the same furnace program, their risk of mechanical damage may differ.

The second design may be more sensitive to defects introduced during machining or handling.

What should technicians look for?

Before milling, check the CAD design for:

Very thin marginal areas

Narrow connectors in multi-unit restorations

Sharp internal corners

Sudden changes in wall thickness

Areas where the tool may have difficulty reaching the intended surface

The minimum thickness and connector dimensions should follow the zirconia manufacturer's instructions and the clinical requirements of the restoration. There is no single minimum value that applies to every zirconia composition, bridge design, and clinical situation.

It is also worth checking whether the milling machine can reproduce the designed geometry accurately. A design may look acceptable on the computer screen, but the actual restoration can contain local defects if the tool cannot access a particular area properly.

5. Handling Before Sintering Is an Often-Overlooked Risk

Before sintering, zirconia restorations are relatively fragile. They have not yet reached their final dense state.

After milling, technicians usually remove the restoration from the disc, separate the support connections, clean the surface, and sometimes make minor adjustments. Each of these operations involves handling.

A crown can be damaged by:

Applying excessive force when removing support connections

Using an unsuitable tool to separate the restoration

Holding a thin marginal area while making adjustments

Dropping the restoration onto a hard surface

Placing several restorations together without adequate protection

The damage may initially be small. A chip at a marginal edge or a crack near a connector may not be immediately obvious.

Technicians should avoid using the thinnest part of the restoration as a gripping point. When separating a crown from its support, they should follow the instructions for the blank and CAM system rather than applying force wherever it is easiest to reach.

If cracks repeatedly appear around the same support-connection areas, the laboratory should review its separation method before changing the furnace program.

A simple comparison test

A laboratory can select several similar crowns and divide them into two groups.

Group A follows the current separation and handling procedure.

Group B follows a revised procedure using a more controlled separation method.

The material batch, CAD design, milling strategy, and sintering program should remain the same.

The laboratory can then compare the number and location of defects before and after sintering.

This is not a substitute for a controlled scientific study, but it can help determine whether handling is contributing to the problem.

6. Moisture and Shading Liquids Should Not Be Ignored

Some zirconia restorations are coloured using liquid shading systems before sintering. Depending on the material and the manufacturer's instructions, the restoration may also be exposed to water or other liquids during processing.

The restoration should not enter the furnace with an uncontrolled amount of liquid remaining on or inside it.

If liquid has penetrated the porous pre-sintered structure, it needs to be removed according to the material manufacturer's instructions. Rapid heating while moisture or liquid remains may create additional problems.

Kuraray Noritake's KATANA Zirconia processing handbook includes moisture absorption and shading-liquid handling among the factors to investigate when restorations develop problems during firing. It advises checking whether the restoration has absorbed too much liquid, including during wet milling or shading.

This does not mean that every coloured crown is at risk of cracking. Many laboratories use shading liquids as part of their normal workflow. The relevant question is whether the liquid, drying procedure, and firing program are compatible with the particular zirconia product.

Practical questions for laboratories

Is the shading liquid approved for the zirconia being used?

Does the supplier specify a drying procedure?

Is the restoration dried for the recommended period?

Are the internal surfaces also checked for remaining liquid?

Does the laboratory use the same firing program for different zirconia products without checking their instructions?

If cracks appear mainly in restorations that have been shaded or processed with liquids, compare them with unshaded restorations from the same batch.

The liquid should not automatically be assumed to be the cause. A comparison can help establish whether the additional processing step is related to the failure.

7. Can the Sintering Process Itself Cause Cracks?

Yes. The thermal process can contribute to cracking, but the conditions need to be identified.

Zirconia is a ceramic material. Like other ceramics, it can develop thermal stresses when different regions of a restoration experience different temperatures at the same time.

A study published in 2023 investigated transient thermal stresses during speed sintering of 3 mol% yttria-stabilized tetragonal zirconia polycrystal (3Y-TZP). The researchers explained that heat moves from the outer surface toward the interior of a solid. This creates temperature gradients, which can produce thermal stresses.

The study showed that faster heating and cooling can increase thermal gradients and the associated transient stresses. Under certain conditions, these stresses may damage the restoration.

The results do not mean that every fast-sintering program will cause cracks. The actual outcome depends on the material, specimen dimensions, furnace conditions, and thermal schedule.

A thin single crown and a large, thick restoration do not have the same thermal behavior. A program validated for one type of zirconia and restoration may not be suitable for another.

What should be checked?

When cracks appear in multiple restorations after firing, review the following:

Is the firing program approved for the zirconia product?

Is the selected program intended for the restoration size and material type?

Has the laboratory changed from one zirconia brand to another without checking the recommended cycle?

Are different materials being processed together under one program?

Do the restorations show similar crack locations or completely different fracture patterns?

One approach is to process a small number of test restorations using the manufacturer's recommended standard program. Keep the milling and handling procedures unchanged.

If the problem continues, the investigation should also cover the material batch and machining process rather than focusing only on the firing schedule.

8. How Can You Identify Where a Crack Started?

Finding a crack is one thing. Identifying its origin is much more difficult.

Visual inspection can show the location of a defect, but it cannot always establish when the defect formed.

For a more useful investigation, the laboratory should record the following information:

Observation Possible area to investigate
Cracks around support connections Separation and handling
Chips or cracks near the internal surface Milling tools and machining strategy
Repeated defects in the same material batch Blank quality and batch consistency
Cracks in very thin or narrow areas CAD design and local geometry
Defects mainly after shading or wet processing Liquid absorption and drying procedure
Several restorations affected in one firing cycle Firing program, loading conditions, and material compatibility

These observations are investigation clues, not definitive diagnoses. A crack near a support connection, for example, may have started during milling and only become visible after sintering.

For difficult cases, fractographic analysis provides more information than visual inspection alone. Researchers examine the fracture surface under magnification to identify the likely fracture origin and the direction in which the crack propagated.

A 2024 study on strength-limiting defects in dental CAD/CAM full-contour zirconia ceramics compared defects associated with milling against defects located within the material. The researchers found that fracture origins differed between the groups. Some specimens failed from external CAM-milling defects, while others showed internal defects such as pores, large grain clusters, and inclusions.

The fracture surface can therefore provide useful evidence. Two crowns may look similar after breaking, but the actual origins of failure may be different.

For routine laboratory work, a microscope and good lighting are useful first steps. For repeated or costly failures, photographs and retained samples can help the material supplier or equipment manufacturer investigate the problem.

9. A Practical Troubleshooting Example

Consider a laboratory that notices several zirconia crowns cracking after sintering over a period of two weeks.

The first reaction might be to lower the sintering temperature. Before changing the program, however, the laboratory should collect some basic information.

Step 1: Check when the defect first appears.

Inspect several restorations immediately after milling, before separation and cleaning. Record any visible chips or cracks.

Step 2: Check the machining process.

Review the bur replacement records and inspect the tools. If the same bur has processed a large number of restorations, compare its condition with that of a new one.

Step 3: Check the material batch.

Record the disc brand, product type, batch number, and manufacturing date, if available. If the problem is limited to one batch, contact the supplier and retain the affected samples.

Step 4: Review the restoration design.

Look for repeated failures around thin margins, connectors, and sharp internal transitions. If several cracks appear in the same type of geometry, review the CAD parameters.

Step 5: Review pre-sintering treatment.

Check whether the affected restorations were shaded, wet-milled, or exposed to cleaning liquids. Confirm that the drying procedure follows the material manufacturer's instructions.

Step 6: Review the firing program.

After collecting the previous information, compare the selected firing cycle with the zirconia manufacturer's recommendations.

This example is an investigation framework, not a documented Zotion customer case. It illustrates why changing the furnace program should not be the only response to a cracking problem.

10. What Should Distributors Know When Customers Report Cracked Crowns?

Distributors often receive complaints before the manufacturer has enough information to identify the cause.

A customer may simply say, "The zirconia cracked during sintering. The material must be defective."

It is understandable that the laboratory would suspect the material, especially when the restoration was intact before firing. However, a useful technical response should gather more information before confirming the cause.

I would suggest asking the customer:

Was the crack visible before sintering?

Which zirconia product and batch were used?

Was the restoration wet-milled or shaded?

Which milling machine and bur set were used?

How many restorations were affected?

Did the cracks appear in the same area?

Was the recommended firing program followed?

Can the laboratory provide photographs of the restoration before and after sintering?

The answers can help distinguish a possible material complaint from a machining or processing issue.

Distributors should also avoid promising that a replacement disc will solve the problem before the cause has been investigated. If the actual issue is a worn bur or unsuitable machining strategy, the same failure may occur again with the replacement material.

For zirconia manufacturers, batch traceability and technical communication are important. A useful complaint record should include the product name, batch number, restoration type, processing conditions, and photographs. When possible, retaining the failed restoration can provide additional evidence.

11. What Can Zirconia Manufacturers Do to Reduce the Risk?

From the manufacturing side, controlling the quality of the blank is only one part of the work.

A zirconia manufacturer should pay attention to several stages.

Powder preparation and forming

Powder dispersion, granule quality, pressing conditions, and density distribution all affect the structure of the blank. Large internal defects formed during pressing may remain after subsequent processing.

Blank inspection

External inspection is useful, but it cannot identify every internal defect. Manufacturers need appropriate process controls and quality checks to monitor consistency between batches.

Material documentation

Flexural strength, translucency, shrinkage factors, and recommended sintering conditions should be communicated clearly. Laboratories need to know which processing parameters apply to each product.

Technical support

When a laboratory reports cracking, the manufacturer should ask about the complete workflow instead of automatically assuming that the furnace or the material is responsible.

For manufacturers and distributors, a complaint can also help identify whether the same issue has appeared in other batches or processing environments.

Conclusion

A zirconia crown that cracks after sintering does not always have a furnace problem. The defect may have started during powder processing, pressing, milling, separation, or pre-sintering treatment. The thermal process may then reveal or extend the damage.

Research has documented machining-related microcracks in the range of 2–15 μm, as well as internal packing defects that are difficult to eliminate through later processing. Other studies have shown that fracture origins can be associated with either external machining damage or defects inside the zirconia material.

For dental laboratories, the most useful approach is to inspect the restoration at several stages and record when the defect first becomes visible. For distributors, collecting batch information, photographs, and processing details is more helpful than immediately attributing every failure to material quality.

A reliable investigation starts with the evidence. Changing the firing program, replacing the zirconia disc, or adjusting the milling machine may all be reasonable actions in certain cases, but the right response depends on where the defect originated.

← Previous: No Information
Send Inquiry